                                  Phone:+86 0537-3330928  
Fax:+86 0537-3330928  
Email :info@darrenco.cn 
  | 
                                 
                              
                            | 
                         
                      
                   
                  
  | 
				  
				  
				  
				  
				  
                
                    
                      
                        
                          
                              
                                
                      
                                
                                  |    WN-1Wide Range Temperature Anodizing Additive  | 
                                 
                                
                                  
                                      
                                        
	
		
			
				This additive is a greenish liquid suitable for the anodization treatment of Al and Al alloy. The H2SO4 anodizing solution with addition of this the additive is featured with the following merits:  
				1. Fast film-formation: the maximum film-formation speed may be reaching 1um/min, specially use in thick-film profile production. 
				2. High productivity: in comparison with the conventional H2SO4 anodizing, solution, the productivity may be increased by 20-40%. 
				3. Wide temperature range for operation: qualified film may be formed, provided temperature is below 35℃. 
				4. The oxide film formed by using this additive is featured by its uniformity in thickness and higher hardness, as well as its better coloring effect and sealing result. | 
		 
		
			| 
				1. Bath Composition (For make-up): | 
		 
		
			| 
				  | 
			
				Sulfuric Acid 
				WN-1 Additive 
				Al3+ 
				Water | 
			
				150±10g/l 
				20-40g/l 
				<20g/l 
				balance | 
		 
		
			| 
				2. Processing Parameters: | 
		 
		
			| 
				  | 
			
				Temperature  
				Current Density 
				Agitation 
				 
				Time 
				  | 
			
				<35℃ 
				1-3.0A/dm2 
				While higher current density is applied, agitation of bath solution should be strengthened, to prevent over heat generated.  
				In accordance with the film thickness requirement, take Tab. 1 shown as below for reference: | 
		 
	
 
	Relation between Film-formation Speed and current Density Tab. 1    
	
		
			
				| 
					Current Density (A/dm2) | 
				
					Film-formation Speed (um/min) | 
			 
			
				
					1.3 
					1.5 
					2.0 
					2.5 
					3.0 | 
				
					0.45 
					0.52 
					0.65 
					0.85 
					1.05 | 
			 
		
	 
	
		  
	
	  
 
                                           | 
                                       
                                    | 
                                 
                                
                                   | 
                                 
                                
                                   | 
                                 
                               
                               | 
                         
                      
                    |